POLYMER CLASS | Polyphenylenes |
COMMON NAMES | Poly(p-xylene), Parylene N , Poly(paracyclophane) |
STRUCTURE BASED NAME | Poly(1,4-phenylene ethylene) |
ACRONYMS | |
CAS # | |
CurlySMILES | C{-}c1ccc(cc1)C{n+} |
CAS # | 1633-22-3 |
COMMON NAMES | p-Cyclophane |
SMILES | C1Cc2ccc(cc2)CCc2ccc1cc2 |
Std. InChI | 1S/C16H16/c1-2-14-4-3-13(1)9-10-15-5-7-16(8-6-15)12-11-14/h1-8H,9-12H2 |
Std. InChIKey | OOLUVSIJOMLOCB-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 94.7 - 99.2 | 99.2 |
Density ρ | g mL-1 | 1.05 - 1.10 | 1.05 |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 333 - 353 | 343 |
Molar Heat Capacity Cp | J (mol K)-1 | 135 | |
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none | 1.47 - 1.67 | 1.57 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 104.15 | |
Van-der-Waals Volume VvW | mL mol-1 | 66.13 | |
Molar Volume Vm | mL mol-1 | 98.2 - 103.5 | 100.5 |
Density ρ | g mL-1 | 1.01 - 1.06 | 1.04 |
Solubility Parameter δ | MPa1/2 | 18.6 - 19.5 | 19.1 |
Molar Cohesive Energy Ecoh | J mol-1 | 35900 - 37400 | 36600 |
Glass Transition Temperature Tg | K | 316 - 354 | 333 |
Molar Heat Capacity Cp | J (mol K)-1 | 126- 141 | 132 |
Entanglement Molecular Weight Me | g mol-1 | 1000 | |
Index of Refraction n | none | 1.57 - 1.65 | 1.59 |