POLYMER CLASS | Epoxy Resin |
COMMON NAMES | Bisphenol-F diglycidyl ether epoxy resin, Poly(Bisphenol F-co-epichlorohydrin) |
STRUCTURE BASED NAME | Poly(1-oxy-2-hydroxytrimethyleneoxy-1,4-phenylene-methylene-1,4-phenylene) |
ACRONYMS | DGEBF |
CAS # | |
CurlySMILES | C{-}C(O)COc1ccc(cc1)Cc2ccc(cc2)O(n+} |
CAS # | |
COMMON NAMES | Bisphenol F diglycidyl ether, Bis(4-glycidyloxyphenyl)methane, |
SMILES | O1C C1COc1ccc(cc1)Cc1ccc(cc1)OC C1O C1 |
Std. InChI | InChI=1S/C20H22O4/c1-14(15-2-6-17(7-3-15)21-10-19-12-23-19)16-4-8-18(9-5-16)22-11-20-13-24-20/h2-9,14,19-20H,10-13H2,1H3 |
Std. InChIKey | PZIZOAOYNGSDLZ-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | > 219 | |
Density ρ | g mL-1 | < 1.17 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 353 | |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 256.3 | |
Van-der-Waals Volume VvW | mL mol-1 | 138.8 | |
Molar Volume Vm | mL mol-1 | 219 | |
Density ρ | g mL-1 | 1.17 | |
Solubility Parameter δ | MPa1/2 | 22.1 - 22.5 | 22.2 |
Molar Cohesive Energy Ecoh | J mol-1 | 107000 - 111000 | 108000 |
Glass Transition Temperature Tg | K | 344 - 364 | 352 |
Molar Heat Capacity Cp | J (mol K)-1 | 294 - 308 | 300 |
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none | 1.56 - 1.62 | 1.59 |
Last updated: September 1, 2016