Poly(tetrafluoroethylene)
CROW logo
Poly(tetrafluoroethylene)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyhaloolefins
COMMON NAMESPoly(tetrafluoroethylene), Poly(tetrafluoroethene), Teflon®, Fluon®, Dyneon™, Hyflon®
STRUCTURE BASED NAME Poly(1,1,2,2-tetrafluoroethylene)
ACRONYMS PTFE
CAS # 9002-84-0
CurlySMILES C{-}(F)(F)C{n+}(F)(F)
 

IDENTIFIERS OF MONOMER(S)

CAS # 116-14-3
COMMON NAMESTetrafluoroethene
SMILES FC(=C(F)F)F
Std. InChI 1S/C2H2F2/c1-2(3)4/h1H2
Std. InChIKey BQCIDUSAKPWEOX-UHFFFAOYSA-N
STRUCTURE
Tetrafluoroethene
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-145.9 - 50.047.9
Density ρg mL-1 2.00 - 2.182.12
Solubility Parameter δMPa1/2 9.4 - 14.012.3
Molar Cohesive Energy EcohJ mol-1 4200 - 97007500
Glass Transition Temperature TgK 388 - 399
200 - 243
392
211
Molar Heat Capacity CpJ (mol K)-188 - 96
51.3
93
51.3
Entanglement Molecular Weight Meg mol-13700 - 56004650
Index of Refraction nnone1.30 - 1.531.36
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 100.01
Van-der-Waals Volume VvWmL mol-1 28.11
Molar Volume VmmL mol-144.8 - 51.947.6
Density ρg mL-1 1.93 - 2.232.10
Solubility Parameter δMPa1/2 9.0 - 15.312.9
Molar Cohesive Energy EcohJ mol-1 4200 - 104007900
Glass Transition Temperature TgK 384 - 385385
Molar Heat Capacity CpJ (mol K)-198 - 100
55
99
55
Entanglement Molecular Weight Meg mol-15300 - 55005400
Index of Refraction nnone1.33 - 1.391.36

  Last updated: June 10, 2017

back to top