Melting Points of Polymers

Polymer Name Tm1
(°C)
Poly(acrylonitrile), syndiotactic 321
Poly(6-aminocaproic acid) 224
PoIy(1-butene), isotactic 124
Poly(caprolactam) 222
Poly(decamethylene adipamide), Nylon 10,6 235
Poly(decamethylene sebacamide), Nylon 10,10 202
Poly(etheretherketone), PEEK 357
Poly(ethylene adipate) 63
Poly(ethylene oxide), PEG 66
Poly(ethylene terephthalate), PET 264
Poly(ethylene), PE 141
Poly(hexamethylene adipamide), Nylon 6,6 272
Poly(hexamethylene sebacamide), Nylon 6,10 224
Poly(hexamethylene suberamide), Nylon 6,8 236
Poly(methyl methacrylate), isotactic 144
Poly(methyl methacrylate), syndiotactic 200
Poly(methylene oxide), POM 172
Poly(4-methylpentene) 243
Poly(propylene), isotactic 179
Poly(styrene), isotactic 242
Poly(styrene), syndiotactic 276
Poly(tetramethylene oxide), PTMO 41, 60
Poly(trans-1,4-butadiene) 98, 144
Poly(vinyl alcohol) 231, 266
Poly(vinyl chloride), PVC 220, 305
Poly(vinyl fluoride) 199
Poly(vinylidene chloride) 202
Poly(vinylidene fluoride) 176
Poly(ω-undecanamide), Nylon 11 187
1The Tms are the average of several experimental values.

Polymer Properties Database

Theromophysical Data

Key data on over two hundred
and fifty polymers.

Polymers Index

Typical Performance

Properties of commercial commodity
and engineering polymers.

Plastics  Index

Physics of Polymers

Physical and mechanical properties
of polymers

Phys. Contents

Chemistry of Polymers

Chemical properties and synthesis
of organic polymers.

Chem. Contents